SolaStay® S1 is incorporated to mitigate the photocatalytic and reactive oxygen species generating activities of oxides, protecting from photodegradation, and so improving sunscreen performance. HallBrite® BHB aids wetting and dispersion of oxides and enhances product feel. This broad-spectrum mineral sunscreen cream was subjected to in vitro analysis and delivered SPF ~42, PFA (PPD) ~18 performance with critical wavelength 378 nm.

Scroll right to view specs →
PhaseINCI Name [INN/USAN] (Other Information)Trade Name% WtFunction
ACaprylic/Capric Triglyceride 10.00Emollient
Ethylhexyl OlivateSENSOLENE®3.00Emollient
Butyloctyl SalicylateHALLBRITE® BHB*5.00Emollient
Tocopheryl Acetate 0.20Antioxidant Agent
Ethylhexyl MethoxycryleneSolaStay® S1*2.00Photostabilizer
Cyclopentasiloxane, Disteardimonium Hectorite, Propylene Carbonate 3.00Feel Modification / Enhancement
Cetyl PEG/PPG-10/1 Dimethicone 2.50Emulsifier
Cetyl Dimethicone 1.00Skin Conditioning Agent
BTitanium Dioxide [Titanium Dioxide], Aluminum Hydroxide (60 nm primary particle size) 3.00UV Filter / Sunscreen Agent
Zinc Oxide [Zinc Oxide], Triethoxycaprylylsilane (30-200 nm primary particle size) 8.00UV Filter / Sunscreen Agent
CBeeswax (Cera Alba) 0.30Thickener (Nonaqueous)
C30-38 Olefin/Isopropyl Maleate/MA Copolymer 0.50Film Former
DWater (Aqua) (deionized) up to 100Volatile Carrier
Disodium EDTA 0.05Chelating Agent
Sodium Chloride 0.50Emulsion Stabilizer
EButylene Glycol 3.00Humectant
Preservative a.n.Preservative

PREPARATIVE PROCEDURE

1To the main vessel add phase A and start mixing, disperse phase B in phase A and heat phase AB to 85°C.
2Add phase C to phase AB and mix well until all are dissolved.
3To a secondary vessel add phase D, start mixing and when fully incorporated start heating to 80°C and add phase E.
4When both phases are homogeneous and at their designated temperatures, start homogenizing phase ABC and slowly add phase DE to it under homogenization.
5Cool batch under continued shear until to desired filling temperature.

PRODUCT CHARACTERISTICS (25°C)

AppearanceOff-white cream
Viscosity (Brk, RVDV-II, T-D, 20 rpm, after 24 h at room temperature; mPa∙s)17,000 - 29,000

*Patented and Patent Pending

The information presented herein is believed to be accurate and reliable, but no warranty or guarantee, expressed or implied, is made regarding the information or the performance of any product. Further, nothing contained herein shall be taken as any inducement or recommendation to use, manufacture or sell that may infringe any patents or any other proprietary rights now or hereafter in existence, nor to imply compliance with any regulatory requirements

The Hallstar Company - 120 South Riverside Plaza Suite 1620 - Chicago, IL 60606-3911 USA

Tel.: 877 427 4255 (International n.: +1 312 385 4494) - Fax: +1 330 929 3616 - E-mail: customerservice@hallstar.com Web Site: hallstar.com